How to Weld H13 (1.2344) & DB6 (1.2714) Steel: Welding Procedure and Repair Guide

Short answer: Yes, H13 and DB6 (1.2714) die steel can both be welded, but there are no shortcuts. Here is how to weld H13 & DB6 die steel in short: preheat the die (300–500°C for H13, roughly 300–400°C for DB6), use a dry filler suited to the job, keep the die hot during welding, cool it slowly and temper it right away. Skip any step and the weld is at serious risk of cracking.
Nobody wants to deal with a cracked die. A deformed forging impression or a cavity full of heat checks is just as unwelcome. The question is the same as usual: scrap or weld? If you decide to weld, this guide shows how to weld H13 & DB6 1.2714 welding die steel so the repair last.
Welding could save the tool. It could also destroy it in just one afternoon, hence why all the people in the tool room have an opinion about it. We offer H13 & DB6 1.2714 welding die steel, which means we approach this issue from the angle of steel. We take into consideration the data sheets offered by the producers of the steel, as well as the welding organizations such as TWI, and questions posed to us by the tool room.
This guide to H13 & DB6 1.2714 welding is general information. Always follow the welding sheet from your steelmaker and filler manufacturer, and a qualified welding procedure for your die.
H13 and DB6 1.2714 welding at a glance
Let us start off with the names, as there seems to be some confusion there. H13 1.2344 welding is the name from the AISI nomenclature. The same steel has the following designations H13 1.2344 welding or X40CrMoV5-1 in the German/EN system, and SKD61 in Japan. DB6 1.2714 welding is the market name for 1.2714 (56NiCrMoV7) in India. This is not an official designation; therefore, insist that it be written 1.2714 on the mill test certificate. Böhler sells roughly the same steel as W500, which is approximately equivalent to AISI L6 and JIS SKT4.
| H13 (1.2344 / SKD61) | DB6 (1.2714 / 56NiCrMoV7) | |
| Steel type | 5% Cr-Mo-V hot work steel | Ni-Cr-Mo-V die block steel |
| Strongest at | Hot strength and heat-checking resistance | Toughness and deep hardening in large sections |
| Typical uses | Aluminium die casting dies, extrusion tooling, forging inserts | Hammer and forging dies, die holders, large blocks |
| Typical preheat | 300–500°C (Uddeholm’s QRO 90 Supreme sheet: 330°C ±25°C) | Roughly 300–400°C |
| Hardened die limit | Never above the last tempering temperature | Same rule |
| After welding | Cool slowly, then temper (Uddeholm: about 25°C below the last temper) | Same logic; confirm with the block maker |
| Typical filler | Low-hydrogen hot work filler | Hot work or hardfacing filler suited to the duty, often layered |
| Weld repair | Well documented, matching fillers widely sold | Possible, with the same discipline as H13; fewer published procedures |
H13 1.2344 welding is suitable when the problems are those of cycling and heat checking just like in case of die casting and extrusion operations. On the other hand, DB6 1.2714 welding is preferred when dealing with impact and large cross sections such as when using hammer dies and die holders. In case of uncertainty on which to choose, give more information to the supplier about the die size and temperature.
Should you weld the die or scrap it?
There is no fixed rule, but these questions help a great deal:
How bad is the damage, and where is it? Surface damage, wear and localized cracks that are superficial can be repaired. However, cracks extending into the block or throughout its entire section or starting from a sharp internal corner or other load-bearing areas are more difficult to repair.
What is the die worth? It should be considered how much money was spent on making it, i.e. the costs of the block itself, the cavity and heat treatment plus waiting time for it. A large block with a cavity can be economically repaired while a small one may not be worth it.
How many repairs has it had? There is no fixed limit, but every repair adds stress and another heat-affected zone. A die that has been welded several times in the same spot deserves scrutiny.
Do you know what the die is? Grade, hardness and heat treatment decide the procedure. If there are no records, test the die before you start welding.
Do you know why it cracked? If the cause is still there, it is not likely that the repair will hold. Look into the design, cooling, heating, and steel quality first.
Can you heat treat it properly? A good repair needs a way to preheat the whole die and to temper the die afterwards. If you cannot do that, hand the job to a specialist or replace the die.
In short: weld where there is localized damage, the cause is known, the grade is known and heat can be controlled. Replace the die when the damage is extensive, the same spot keeps failing, or proper heat treatment is not possible
What kind of damage are you repairing?
Cracks, wear and heat checks are all called “repair”. Each is a different job.
Cracks. Cut out the crack completely. TWI advises machining out the defect and leaving a smooth groove with no sharp corners. Check the groove with dye penetrant or magnetic particle testing until it is clean, then clean and dry it. Welding over a crack only hides it.
Worn or deformed impressions. Treat these as layered build-ups. On working surfaces, TWI says the deposit should have the same hardness as the parent metal. In forging impressions some shops cover only the parts most likely to fail rather than filling the entire gap.
Heat checks. Machine out the fine surface networks down to clean metal before welding. If the network is deep and covers most of the cavity, ask whether a new die is needed, and check cooling and warm-up before blaming the steel.
H13 1.2344 welding and repair
H13 steel has 5% chromium and around 0.4% carbon. H13 1.2344 welding steel is the material from which aluminium die casting dies, extrusion tooling and forging inserts are made. This is due to the fact that it retains its mechanical properties in a heated state and is resistant to heat checking.
H13 1.2344 welding is also crack-prone when welded. As per TWI, the carbon equivalent of tool and die steels makes them highly susceptible to cracking. Welded areas cool off quickly, resulting in hard and brittle martensite. Residual stress or presence of any hydrogen content can result in cracking.
Annealed or hardened?
Weld the H13 1.2344 welding in the annealed state wherever possible before hardening and tempering the die. This is what TWI suggests. Welding can also be done on a hardened and tempered die, but preheating or tempering should not be carried out at temperatures higher than the prior tempering temperature.
What preheat should you use?
There is quite a variance among the published numbers regarding this issue. According to West Yorkshire Steel, 300-500°C is the proper preheat temperature for H13 1.2344 welding. The recommended welding temperature of QRO 90 Supreme, provided by Uddeholm, is 330°C ±25°C. However, do remember that QRO 90 Supreme is just another high-alloyed hot work steel. Uddeholm’s welding recommendation for Orvar Supreme (their grade H13) in the company’s general welding brochure provides a minimum preheat of 300°C for TIG welding. A Castolin recommendation provides 200°C for TIG welding.
This range is not a mistake. It is a reflection of die size, condition and filler metal. Follow the recommendations of the welding sheet.
The repair, step by step
- Know the die. Verify the grade, hardness, and heat treatment. In case someone did not document these, perform tests prior to welding.
- Cut out the whole defect. Remove any nitrided layer first. Leave a smooth contour with no sharp edges, confirm it is defect-free with dye penetrant or magnetic particle testing, then clean and dry the groove.
- Preheat slowly and keep it there. Heat the whole die evenly and hold the temperature through the job. See the heating section below for how.
- Choose the process and filler. Use dried, low-hydrogen consumables with a hot work filler. For a cavity that will be polished or photo-etched, Uddeholm wants a filler that matches the base composition.
- Weld short beads. Keep heat input low, clean between passes and leave a few minutes between layers. Where possible, peen the weld and reverse the welding direction by 180° between layers.
- Cool slowly, then temper without delay. Cool at 20–40°C per hour for the first two hours, air cool to below 70°C, then temper for two hours. Where the weld metal tempers the same way as the base metal, Uddeholm tempers at about 25°C below the die’s previous tempering temperature, so the base steel does not soften. TWI likewise says post-weld heat treatment should start immediately after welding. A newly welded die should never spend the night in a cold corner of the workshop. If the die was welded in the annealed state, anneal it, then harden and temper it normally.
- Finish and test. Finish the repair work, test for cracks and check hardness in the weld area, heat affected area and base steel. Heat the die up correctly before putting it back into use.

Welding without pulling the die from the machine
It is done in some shops. Uddeholm does not recommend it. If there is truly no alternative, its welding sheets describe a last-resort procedure that includes a second heating step after welding. Follow the sheet for your exact steel, and expect a less reliable repair than a full furnace cycle.
Expect a slightly weaker repair
According to a Daido Steel report on die casting repair, the weld material is somewhat weaker and more susceptible to heat-checks than the original steel, but good post-welding heat treatment can restore some of its properties. Be ready for the welded area to show up first during the next inspection.
DB6 (1.2714) welding and repair
The designation used for 1.2714 steel in India is DB6. It corresponds to 56NiCrMoV7 steel in the DIN and EN system. The composition is entirely different from H13; 0.55% carbon, 1.1% chromium, 1.7% nickel and small amount of molybdenum and vanadium. The carbon gives DB6 high hardness and strength, while the nickel supports toughness. Together they handle heavy impact well, which means that it can withstand a lot of impact. This property makes it suitable for hammer dies, forging dies, die holders and large blocks.
At that carbon level, the weld and heat-affected zone form very hard, brittle martensite if they cool too fast. Slow cooling and prompt tempering matter as much here as with H13 1.2344 welding. There are two varieties of DB6 1.2714 welding: soft annealed (hardness up to 248 HB according to EN ISO 4957 standard) and quenched and tempered (about 370–415 HB, approximately 39–43 HRC).
With many blocks arriving already hardened, many DB6 1.2714 welding repairs involve welding hard steel, so standard procedure is to preheat to a temperature below the last tempering process, and then retemper following the welding. Ask your supplier for the final tempering temperature of the block prior to preheating.
Preheat and filler for DB6 1.2714 welding
Guidance and experience range between 300-400°C in relation to DB6 1.2714 Welding. Don’t heat above the previous tempering temperature of the die and maintain the temperature throughout the procedure.
When selecting filler metals, forging-die repairs can be done using multi-pass buildup and the selection of appropriate metal will depend on whether the application is one of impact resistance or abrasion or a combination of the two. Check with your steel/filler manufacturer for the best metal to use with your particular die. Some companies don’t even build up the entire impression and instead build up the areas where failures are likely to occur using hard facing rods (iron or cobalt alloy).
Cooling, tempering and warm-up
Cooling and tempering schedules for DB6 1.2714 Welding depend on block size, delivery condition and filler, so take them from the block maker’s welding sheet. The principles match H13 1.2344 welding: cool slowly, temper promptly and stay below the last tempering temperature. Because DB6 carries more carbon, do not simply copy an H13 schedule onto it. Large blocks need an experienced heat treater and a furnace. If you are unsure, send us the block size, condition and job details and we will help.
Forging dies too should be properly warmed before re-introduction into production. The repaired die should never encounter its first hot billet in a cold state. Warm up to your normal preheat temperature for the die, and find the appropriate temperature from the forging process engineer or steel supplier.
Heating and temperature control
A lot of failed repairs trace back to heat control rather than the welding itself.
How to heat. The furnace offers the best way of heating the entire block uniformly. Gas burners, electric heating blankets, and ceramic pad heaters are options for large blocks. However, heating should be as uniform as possible. Heating using a torch on one end of the block will build up stress and not eliminate it.
How to check temperature. Thermocouples attached to the die, pyrometers, or temperature-indicating crayons are methods used. Infrared temperature guns give incorrect results when working with smooth or scaled steel. It is important to use several different areas, even some on the opposite side of where the heating occurs.
Soak. Hold the die until the whole section, not just the surface, has reached the preheat temperature. Ask the block maker or your heat treater for the soak time for your block size.
Interpass. The data sheet for Uddeholm’s welding sheets specifies that the temperature around the weld must not exceed 150°C beyond the preheat temperature; otherwise, the base material might soften or crack. Fillers also have their own maximum interpass temperature, which can be seen on the electrode/rod data sheet.
Keep it warm, don’t let drafts get to it. Protect the die from the elements and keep the shop door closed when doing the work so that it could be done in one operation. Otherwise consult your welding engineer about stop procedures.

Stick, TIG or laser: which process?
| Process | Best for | Heat input | Watch out for |
| Stick (MMA/SMAW) | Build-ups and larger repairs. TWI notes it is popular because equipment and consumables are easy to find. | Higher than TIG or laser | Electrodes must be dried and kept dry. More heat means tighter interpass control. |
| TIG (GTAW) | Cavities, edges and fine detail. It gives the most control. Rods made for H11, H12 or H13-type repair are a common choice. | Lower than stick | Needs a skilled welder. Slow for big build-ups. |
| Laser | Small, precise repairs. TWI says it uses low heat input. | Very low | Usually a specialist service. Uddeholm’s brochure lists its laser filler with no preheat and a two-hour temper at 250°C, but follow your repair provider’s procedure. |
Whatever the process, the basics do not change: clean the area, dry the consumables, control the temperature and temper afterwards.
Choosing the filler
Filler material according to application. Regarding working surfaces, TWI recommends filler material to have hardness similar to the base material. There are other types of filler materials which are used in non-critical areas.
Composition matching for polished cavities. In case the cavity has to undergo polishing or photo-etching process, Uddeholm suggests filler material that has same composition as the base material.
Low-hydrogen and dry. Store electrodes either in their packs or in a desiccator until you start to weld them and ensure that they are clean and dry prior to welding since wet electrodes cause hydrogen to get into the joint.
Example. Uddeholm’s QRO 90 Weld is a basic coated electrode and QRO 90 TIG-Weld is a TIG rod. They are recommended by Uddeholm for its hot work steels such as Orvar Supreme. Check the datasheet for as-welded hardness and tempering. Filler manufacturers produce their own equivalents. Always choose the filler for your specific steel.
Buffer layers and hardfacing. There are a number of techniques used where the soft buffer layer is deposited below the hard layer so as to minimize the chance of cracking while some particular regions are hardfaced with the use of certain hardfacing alloys. Please inform your filler manufacturer in case you require this treatment for your steel application.
Describe your application to the filler manufacturer. The casting, extruding, or forging of the part will affect your repair differently. Inform your filler manufacturer what you are doing.
Hardness after welding
In fact, the hardness of hot work filler weld deposits is usually quite high as deposited, which means it is often around 50-55 HRC depending on the filler, while tempering decreases the hardness of those deposits to the required working hardness. For aluminium die casting dies, the working hardness is typically in the mid-40s to low-50s HRC, depending on the steel and application; check your steelmaker’s datasheet. Blocks DB6 1.2714 welding can be ordered in hardness 39-43 HRC. 1.2714 welding
Measure hardness at three places: the weld metal, the heat-affected zone and the base steel. A portable hardness tester works on the repaired die. A heat-affected zone softer than the base steel suggests the die was heated above its last tempering temperature. A weld much harder than the base steel may point to under-tempering. Measure rather than assume.
Troubleshooting weld problems
| What you see | Likely causes | What to try |
| Crack in or beside the weld soon after welding | Preheat too low or lost, cooling too fast, damp consumables, defect not fully removed | Check temperature records, dry the consumables, cut out the crack completely and re-weld to a proper schedule |
| Cracks that show up hours or days later | Hydrogen and residual stress, too long a gap before tempering | Dry consumables, cool slowly, temper promptly |
| Porosity or gas pores | Damp electrodes, grease, coolant or nitrided case left in the groove, poor gas cover in TIG | Clean, dry and re-grind the area; check shielding gas |
| Soft spot beside the weld | Base steel went above its last tempering temperature, interpass too high | Check temperatures; the area may need re-heat treatment |
| Weld lifts or spalls in service | Poor fusion, damaged metal left behind, filler too hard or too brittle for the duty, cold start | Re-check the groove preparation and the filler; warm the die up before production |
| Same spot keeps cracking | The root cause is still there | Look at die design, sharp corners, cooling, warm-up and steel quality before welding again |
| Dimensions drift after repair | Uneven heating, heavy heat input, re-hardening | Leave machining allowance, balance the heat, and finish machining after the final heat treatment |
Best practices and safety
- Clean first. Grease, scale, coolant, and nitrided surface can cause porosity and cracks. Never weld through a nitrided surface; grind out the nitrided layer at the area of repair and re-nitride after repair if the process requires it.
- Dry your consumables. Wet electrodes and rods will introduce hydrogen into the weld metal.
- Preheat all the way. Preheat uniformly; maintain constant interpass temperature; avoid draft cooling during welding operation.
- Write it down. Document the values of preheat, filler, temper and hardness. Then you can start the next repair with the information rather than relying on memory.
- Find out the root cause. In case of a recurrent problem, investigate die design, cooling, heating up and steel grade before you start welding.
- Treat the heat with respect. At 300-500°C the die can look cool enough to touch and still burn severely. Use adequate PPE, mark hot dies with appropriate signs, use adequate hoisting devices, and have a fire watch.
- Breathe clean air. Fumes from alloy filler and tool steel, in particular chromium and nickel, should not be inhaled. Maintain fume exhaust, and read the SDS for the filler you are using.
Buying the right steel before you weld
Good repairs start with good steel. DB6 1.2714 welding a trade name, not a formal standard, so buy on the mill test certificate, not on a listing title. Ask for:
- Grade and standard. 1.2344 or 1.2714 on the certificate, not only the trade name. If 1.2714 – compare the certificate’s chemical analysis with EN ISO 4957 specifications. The allowed limits for H13 steel are slightly different from one standard to another, compare the certificate to the standard indicated on the drawing.
- Delivery condition and hardness. For DB6 1.2714 Welding, soft annealed means a maximum of 248 HB per EN ISO 4957. Quenched and tempered is a supplier range, commonly around 370-415 HB near the surface. State the exact hardness range and your block size on the order.
- Grade of steel for die casting. NADCA #207 establishes Grade A (Premium, conventional melting H13 steel) and Grade B (Superior, re-melting H13, e.g. ESR). If your die will be used for aluminium die casting – specify which grade you need and make sure that the certificate mentions it. Also make sure what edition of NADCA #207 your customer specifies.
- Testing and Traceability. Ask for batch traceability, ultrasonic test reports for blocks, and a named contact who can answer your welding and heat-treatment questions.
- Annealed or pre-hardened steel. You should choose annealed steel when you want to perform welding, stress relieving, and hardening of material as you need significant repair and build-up work. Prehardened steel saves the step of heat treatment and limits preheat temperature.

Why buy from Virat Special Steels
H13 & DB6 1.2714 welding Die Steel is available from Virat Special Steels in form of sheet, round, square and blocks. The mill test certificate, batch traceability and ultrasonic test certificate for blocks are provided along with block cutting service. Please inform us regarding application of the job, die size and temperature of job and our metallurgist will help in selecting correct grade.
Frequently asked questions
Can H13 steel be welded? Yes. H13 1.2344 welding can be done both in an annealed state and a hardened one, but the material cracks without appropriate precautions. Preheat the steel, select an adequate low hydrogen filler, maintain a constant inter pass temperature, cool slowly and temper the steel immediately. Make sure you adhere to your steelmaker’s welding sheet.
What preheat temperature should I use for H13? Published guidance is commonly 300-500°C, and some filler makers allow lower for TIG. Hold the temperature during the whole welding process. Uddeholm gives a minimum of 300°C for TIG welding Orvar Supreme. If the material is a hardened die, do not exceed its tempering temperature. Verify this value according to the data sheets for the specific steel and filler used.
Can I weld H13 without preheating? Not with arc welding. Preheat slows cooling and reduces the risk of brittle martensite and hydrogen cracking in the weld zone. Laser repair is different: Uddeholm lists a laser filler with no preheat, but with a tempering treatment afterwards.
Can DB6 (1.2714) be welded? Yes. DB6 1.2714 welding carries about 0.55% carbon, so it hardens easily and can crack if it cools too fast. Preheat to roughly 300–400°C, keep the temperature steady, cool slowly and temper promptly, following the steel maker’s welding sheet.
What is the equivalent of DB6 steel? DB6 steel is 1.2714 (56NiCrMoV7). The Böhler equivalent for this steel is W500, which is said to be equivalent to about AISI L6 and JIS SKT4. Because DB6 is not a standardised name, always order it as 1.2714.
What is DB6 used for? Hammer dies, forging dies, die holders and die blocks.
Is H13 the same as 1.2344 and SKD61? Yes, all are equivalent designations. H13 is AISI designation, while 1.2344 and X40CrMoV5-1 are German and EN designations respectively, and SKD61 is Japanese designation. Compositional tolerances vary somewhat from system to system, so if your drawing specifies one of these grade names, please refer to the certificate for its exact content.
What is the difference between H13 and DB6? H13 is a 5% chromium hot work steel developed for good hot strength and resistance to heat checking. DB6 1.2714 welding is a nickel-chromium-molybdenum-vanadium steel, developed for toughness and good hardenability in thick sections.
Which filler rod should I use for H13 repair? Select a low-hydrogen hot work tool steel filler rod depending on your requirement. For polished or photo-etched cavities, select a filler rod that is compatible with the base material. Welding rods used for repairing H11, H12 or H13 are commonly used. Inform the manufacturer of the filler rod regarding the type of die (casting, extrusion or forging) so they may suggest the suitable filler rod.
Is TIG, stick or laser welding better for die repair? The most preferred is TIG for cavity welds and details. Manual metal arc welding or stick welding is appropriate for build-up welds. As per TWI, laser welding is suitable for precise welding with low heat input.
Can I weld a hardened die without annealing it? Yes, but the guidelines are different. Make sure that the preheat and post-weld temper are lower than the final tempering temperature of the die so that the base steel is not softened. Still, TWI recommends annealing for welding whenever possible, especially for larger repairs which will be subsequently hardened.
Do I have to temper after welding? Yes. The weld metal and the heat affected zone will remain in the hardened state and thus become brittle and retain high levels of residual stresses. After welding a hardened die, cool slowly and then temper immediately at about 25°C below its final tempering temperature (based on Uddeholm guidelines where the weld metal has tempering properties equal to those of the base). After welding an annealed die, anneal, harden and temper it normally like in a heat treatment cycle.
What hardness should a repaired die have? Hot work filler deposits are very hard as welded, often around 50-55 HRC depending on the filler. Tempering brings the repair down to working hardness. For aluminium die casting dies this is typically in the mid-40s to low-50s HRC, depending on the steel and application, so check your steelmaker’s datasheet. Measure hardness in the weld metal, the heat-affected zone and the base steel.
Can I weld a nitrided die? It cannot be done in the nitrided zone. First, remove it by grinding. This is necessary to avoid cracks and porosity when welding through the case. Re-nitride if required afterwards.
How many times can a die be repaired? It depends. The number of repairs that you undertake will add up the stresses and heat affected zones in each case. If you find that there is repeated cracking in the same area of the die, then consider looking into the design of the die, the cooling process, preheating and the quality of the steel.
Should I choose H13 or DB6 for my die? Select H13 when thermal cycling and heat checking become the major concern, like aluminium die casting and extrusion dies. Select DB6 when impact and cross-sectional size become the major concern, like hammer dies and die holder dies.
Conclusion
A welded die can give a long service life, or it can fail on its first run. The difference is rarely luck. It comes from knowing the steel grade, preheating the whole die, choosing the right filler, and controlling cooling and tempering. Start with known steel and the whole job becomes much simpler.
Require H13 or DB6 die steel for your dies and repair projects? Request a quote from Virat Special Steels and expert advice on how best to meet your needs. Get in touch with us at our metallurgical division for certificates, ultrasonic testing data or even cut-to-size blocks of steel.